高清有码中文字幕I在线观看中文字幕亚洲I欧美性XXXX极品少妇I国产最新在线观看I欧美久热I色二区I97视频久久久I精品国产欧美一区二区I色约约一区=区三区I丝袜阁I亚洲无码久久久久I精品色导航I亚洲天堂2027I97人成视频在线IXXX国产精品午XXXI超碰最新网址I午夜男人影院I久久亚洲婷婷

Common problems and solutions of composite membrane

Common problems and solutions of composite membrane

2022-12-05

Common problems and solutions of composite membrane:

1、 The following three treatment methods are tested for poor adhesion due to insufficient oxidation of the resin surface:

1. Add air gap interval properly;

2. Reduce the winding speed of the extruded composite film;

3. Equipment ozone generator.

The adhesion force is generally related to the surface oxidation degree (according to the resin temperature, air volume and residence time) and viscosity (according to the temperature and resin type).

Generally, when extruding at the same temperature and at the same extrusion rate, decreasing the film thickness or advancing the winding rate will reduce the adhesion. Even at the same set temperature, the forward extrusion rate may also reduce the resin temperature and adhesion (but the degree and tendency may vary according to the characteristics of the extruder and the type of heating equipment). At the same processing temperature, the degree of oxidation will also vary with the type of extrusion coating. In general, the higher the melt index, the lower the density, the more oxidation tendency.

2、 The temperature when the resin is pressed against the substrate is too low. The following three treatment methods are tested:

1. Advance the resin temperature to fully plasticize and mix the resin. The higher the heating temperature of the compression section and homogenization section, the higher the degree of resin plasticization and mixing, but the higher the temperature, the easier the resin differentiation. The heating temperature shall be set according to the resin type and its melt index.

2. Do not make the orientation of the die mouth too close to the side of the cooling roller to avoid the resin from being too cooled before pressing onto the substrate.

3. Preheat the substrate through the oven.